Chemical composition

wt% · log scale
0.010.1110100Cr0.06 – 0.2Cu0.1Fe0.15Mg0.6 – 0.8Mn0.1Si0.15Ti0.1 – 0.2Total Each0.05Total Others0.15Zn6 – 7
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2240 MPaTensile strength Rm310 MPaElongation A10 %sand castings, solution heat treated artificially agedYield strength Rp0.2220 MPaTensile strength Rm275 MPaElongation A7 %sand castings +F

Chemical composition

ElementminmaxSimilarRemarks
Al​​Bal​​
Cr0.060.2
Cu0.1
Fe0.15
Mg0.60.8
Mn0.1
Si0.15
Ti0.10.2
Total Each0.05
Total Others0.15
Zn67

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
sand castings, solution heat treated artificially aged24031010
sand castings +F2202757