中国 · CNS

3003

CNS H 3025:2009 — Aluminium and aluminium alloy sheets and plates

化学成分

元素minmax相似备注
Al​​Bal​​​​Bal​​
Cu0.050.2
Fe0.7
Mn11.5
Others Total0.05
Si0.6
Total Others0.15
Zn0.1

力学性能

热处理 / 状态屈服强度抗拉强度伸长率断面收缩率冲击功硬度
厚板, 薄板  Annealed (O)   > 0,2 mm,63 <= 136.0096.0022.00
厚板, 薄板  Annealed (O)   > 0,32 mm,15 <= 036.0096.0014.00
厚板, 薄板  Annealed (O)   > 0,63 mm,32 <= 036.0096.0020.00
厚板, 薄板  Annealed (O)   > 1,3 mm,2 <= 636.0096.0025.00
厚板, 薄板  Annealed (O)   > 6,3 <= 80 mm3696 132.0023
厚板, 薄板  Strain-hardened - 3/4 hard (H16)  > 0,2 mm,63 <= 1147.00168.003.00
厚板, 薄板  Strain-hardened - 3/4 hard (H16)  > 0,32 mm,15 <= 0147.00168.001.00
厚板, 薄板  Strain-hardened - 3/4 hard (H16)  > 0,63 mm,32 <= 0147.00168.002.00
厚板, 薄板  Strain-hardened - 3/4 hard (H16)  > 1,2 <= 4 mm147168 208.004
厚板, 薄板  Strain-hardened - 4/4 hard (H18)  > 0,2 mm,63 <= 1168.00188.002.00
厚板, 薄板  Strain-hardened - 4/4 hard (H18)  > 0,32 mm,15 <= 0168.00188.001.00
厚板, 薄板  Strain-hardened - 4/4 hard (H18)  > 0,63 mm,32 <= 0168.00188.001.00
厚板, 薄板  Strain-hardened - 4/4 hard (H18)  > 1,2 mm,2 <= 3168.00188.004.00
厚板, 薄板  只应变硬化 (H112)  > 12,5 <= 40 mm4110710
厚板, 薄板  只应变硬化 (H112)  > 40 <= 80 mm≤41≤102≤16
厚板, 薄板  只应变硬化 (H112)  > 6,5 mm,3 <= 1271.00117.008.00
厚板, 薄板  应变硬化 - 1/2 硬 (H14)  > 0,2 mm,63 <= 1117.00142.003.00
厚板, 薄板  应变硬化 - 1/2 硬 (H14)  > 0,32 mm,2 <= 0117.00142.001.00
厚板, 薄板  应变硬化 - 1/2 硬 (H14)  > 0,63 mm,32 <= 0117.00142.002.00
厚板, 薄板  应变硬化 - 1/2 硬 (H14)  > 1,3 mm,2 <= 6117.00142.005.00
厚板, 薄板  应变硬化 - 1/2 硬 (H14)  > 6,3 <= 25 mm117142 183.008
厚板, 薄板  应变硬化 - 1/4 硬 (H12)  > 0,2 mm,63 <= 189.00122.004.00
厚板, 薄板  应变硬化 - 1/4 硬 (H12)  > 0,63 mm,4 <= 086.00122.003.00
厚板, 薄板  应变硬化 - 1/4 硬 (H12)  > 1,3 mm,2 <= 686.00122.006.00
厚板, 薄板  应变硬化 - 1/4 硬 (H12)  > 6,3 <= 50 mm86122 162.009