国际标准 · ISO
6101
ISO 6362-2:2012 — Wrought aluminium and aluminium alloy extruded rods/bars, tubes and profiles - Part 2: Mechanical properties
力学性能
| 热处理 / 状态 | 屈服强度 | 抗拉强度 | 伸长率 | 断面收缩率 | 冲击功 | 硬度 |
|---|---|---|---|---|---|---|
| Extruded bars, rods 固溶热处理和人工时效(T6) 17 mm <= D or S <= 30 mm | ≤145 | ≤175 | ≤14 | |||
| Extruded bars, rods 固溶热处理和人工时效(T6) 3 mm <= D or S <= 7 mm | ≤165 | ≤195 | ≤10 | |||
| Extruded bars, rods 固溶热处理和人工时效(T6) 7 mm <= D or S <= 17 mm | ≤165 | ≤195 | ≤12 | |||
| Extruded bars, rods 固溶热处理和人工过时效(稳定) (T7) 3 mm <= D or S <= 17 mm | ≤110 | ≤135 | ≤10 | |||
| Extruded tubes 固溶热处理和人工时效(T6) 12 <= t <= 16 mm | ≥145 | ≥175 | ≥14 Lo = 50mm | |||
| Extruded tubes 固溶热处理和人工时效(T6) 3 <= t <= 12 mm | ≥165 | ≥195 | ≥10 Lo = 50mm | |||
| 挤压异型材 Solution heat treated and overaged/stabilized (T7) 3 <= t <= 17 mm | ≥110 | ≥135 | ≥10 Lo = 50mm | |||
| 挤压异型材 固溶热处理和人工时效(T6) 17 < t <= 30 mm | ≥145 | ≥175 | ≥14 Lo = 50mm | |||
| 挤压异型材 固溶热处理和人工时效(T6) 3 < t <= 7 mm | ≥165 | ≥195 | ≥10 Lo = 50mm | |||
| 挤压异型材 固溶热处理和人工时效(T6) 7 < t <= 17 mm | ≥165 | ≥195 | ≥12 Lo = 50mm |