英国 · B.S.
S 420 ML
BS EN 10113-3 — 可焊接细晶粒结构钢热轧产品 - 第3部分:热机械轧制钢的交货条件。
化学成分
wt% · 对数刻度- min – max 范围
- 典型值
力学性能
按热处理状态分组化学成分
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| Al | 0.02 | If sufficient other nitrogen binding elements are present | ||
| C | 0.16 | For long products | ||
| Cr | ||||
| Cr+Cu+Mo | Cr+Cu+Mo < 0.6% | |||
| Mn | 1.7 | |||
| Mo | 0.2 | |||
| N | 0.02 | |||
| Nb | 0.05 | |||
| Ni | 0.3 | For long products | ||
| P | 0.03 | |||
| S | 0.025 | For railway applications a maximum S content of 0 | ||
| Si | 0.5 | |||
| Ti | 0.05 | |||
| V | 0.12 |
力学性能
| 热处理 / 状态 | 屈服强度 | 抗拉强度 | 伸长率 | 断面收缩率 | 冲击功 | 硬度 |
|---|---|---|---|---|---|---|
| Flat products 热机械轧制 <= 16 mm | ≥420 Yield stress is Upper Yield Stress (Reh) | 500–660 | ≥19 For t < 3 mm | ≥40 Charpy V Notch (+20°C) (trans.);≥63 Charpy V Notch (+20°C) (long.) | ||
| Flat products 热机械轧制 > 16 <= 40 mm | ≥400 Yield stress is Upper Yield Stress (Reh) | 500–660 | ≥19 For t < 3 mm | ≥40 Charpy V Notch (+20°C) (trans.);≥63 Charpy V Notch (+20°C) (long.) | ||
| Flat products 热机械轧制 > 40 <= 63 mm | ≥390 Yield stress is Upper Yield Stress (Reh) | 500–660 | ≥19 For t < 3 mm | ≥40 Charpy V Notch (+20°C) (trans.);≥63 Charpy V Notch (+20°C) (long.) | ||
| 长材 热机械轧制 <= 16 mm | ≥420 Yield stress is Upper Yield Stress (Reh) | 500–660 | ≥19 For t < 3 mm | ≥40 Charpy V Notch (+20°C) (trans.);≥63 Charpy V Notch (+20°C) (long.) | ||
| 长材 热机械轧制 > 16 <= 40 mm | ≥400 Yield stress is Upper Yield Stress (Reh) | 500–660 | ≥19 For t < 3 mm | ≥40 Charpy V Notch (+20°C) (trans.);≥63 Charpy V Notch (+20°C) (long.) | ||
| 长材 热机械轧制 > 40 <= 150 mm | ≥390 Yield stress is Upper Yield Stress (Reh) | 500–660 | ≥19 For t < 3 mm | ≥40 Charpy V Notch (+20°C) (trans.);≥63 Charpy V Notch (+20°C) (long.) |