德国 · DIN
1.0566
DIN EN 10217-3:2005 — 承压焊接钢管 - 交货技术条件 - 第3部分:细粒合金钢管
化学成分
| 元素 | min | max | 相似 | 备注 |
|---|---|---|---|---|
| Al | 0.02 | Al/N=>2 | Al/N=>2 | |
| C | 0.18 | |||
| Cr | 0.3 | |||
| Cr+Cu+Mo | 0.45 | The sum of the percentage by mass of the three elements Cr | The sum of the percentage by mass of the three elements Cr | |
| Cu | 0.3 | |||
| Mn | 0.9 | 1.7 | ||
| Mo | 0.08 | |||
| N | 0.02 | |||
| Nb | 0.05 | |||
| Nb+Ti+V | 0.12 | |||
| Ni | 0.5 | |||
| P | 0.025 | |||
| S | 0.02 | |||
| Si | 0.5 | |||
| Ti | 0.03 | |||
| V | 0.1 |
力学性能
| 热处理 / 状态 | 屈服强度 | 抗拉强度 | 伸长率 | 断面收缩率 | 冲击功 | 硬度 |
|---|---|---|---|---|---|---|
| 焊接钢管 正火(N) 12 < T <= 20 mm | ≥355 or Upper yield stress | 490–650 | ≥22 Long. | |||
| 焊接钢管 正火(N) 20 < T <= 40 mm | ≥345 or Upper yield stress | 490–630 | ≥22 Long. | |||
| 焊接钢管 正火(N) T <= 12 mm (t - 壁厚) | ≥355 or Upper yield stress | 490–650 | ≥22 long. test | |||
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | ≥47 KV (20°C);≥43 KV (0°C);≥39 KV (-10°C);≥35 KV (-20°C);≥31 KV (-30°C);≥27 KV (-40°C);≥70 KV (20°C);≥65 KV (0°C);≥60 KV (-10°C);≥53 KV (-20°C);≥47 KV (-30°C);≥40 KV (-40°C) |
高/低温力学性能
| 热处理 / 状态 | 温度 ℃ | min | 备注 |
|---|---|---|---|
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | -10 | 39 | KV |
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | -20 | 35 | KV |
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | -30 | 31 | KV |
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | -40 | 27 | KV |
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | -10 | 60 | KV |
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | -20 | 53 | KV |
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | -30 | 47 | KV |
| 焊接钢管 正火(N) T <= 16 mm (T <= 40 mm) 用于高频焊接(HFW)钢管 (用于SAW钢管) | -40 | 40 | KV |