法国 · AFNOR NF
S 550 Q
NF EN 10025-6 — 热轧结构钢产品 - 第6部分:平板产品的高屈服强度结构钢在淬火和回火状态下的交货技术条件。
化学成分
| 元素 | min | max | 相似 | 备注 |
|---|---|---|---|---|
| Al | 0.013 | The minimum grain-refining element content of 0 | The minimum grain-refining element content of 0 | |
| B | 0.006 | |||
| C | 0.22 | |||
| CEV | 0.65 | For product thickness t <= 50 mm; for product thickness 50 < t <= 100 mm CEV=0.77%; for product thickness 100 < t <= 150 mm CEV=0.83%. | For product thickness t <= 50 mm; for product thickness 50 < t <= 100 mm CEV=0.77%; for product thickness 100 < t <= 150 mm CEV=0.83%. | |
| Cr | 1.6 | |||
| Cu | 0.55 | |||
| Mn | 1.8 | |||
| Mo | 0.74 | |||
| N | 0.016 | |||
| Nb | 0.07 | |||
| Ni | 2.1 | |||
| P | 0.03 | |||
| S | 0.017 | |||
| Si | 0.86 | |||
| Ti | 0.07 | |||
| V | 0.14 | |||
| Zr | 0.17 |
力学性能
| 热处理 / 状态 | 屈服强度 | 抗拉强度 | 伸长率 | 断面收缩率 | 冲击功 | 硬度 |
|---|---|---|---|---|---|---|
| 厚板和宽扁钢 淬火和回火 | ≥27 Charpy V Notch; -20°C; (trans.);≥30 Charpy V Notch; 0°C; (trans.);≥30 Charpy V Notch; -20°C; (long.) | |||||
| 厚板和宽扁钢 淬火和回火 > 100 <= 150 mm | ≥490 Yield stress is Upper Yield Stress (Reh) | 590–770 | ≥16 Lo = 5 | ≥40 Charpy V Notch; 0°C; (long.) | ||
| 厚板和宽扁钢 淬火和回火 > 50 <= 100 mm | ≥530 Yield stress is Upper Yield Stress (Reh) | 640–820 | ≥16 Lo = 5 | ≥40 Charpy V Notch; 0°C; (long.) | ||
| 厚板和宽扁钢 淬火和回火 >= 3 <= 50 mm | ≥550 Yield stress is Upper Yield Stress (Reh) | 640–820 | ≥16 Lo = 5 | ≥40 Charpy V Notch; 0°C; (long.) |
高/低温力学性能
| 热处理 / 状态 | 温度 ℃ | min | 备注 |
|---|---|---|---|
| 厚板和宽扁钢 淬火和回火 | -20 | 27 | Charpy V Notch; trans. |